Influence of alloying elements on as-cast microstructure and strength of gray iron

被引:71
|
作者
Xu, W
Ferry, M [1 ]
Wang, Y
机构
[1] Univ New S Wales, Sch Mat Sci & Engn, Sydney, NSW 2052, Australia
[2] Xian Univ Technol, Dept Mat Sci & Engn, Xian, Peoples R China
关键词
gray cast iron; microstructure; casting; ausferrite;
D O I
10.1016/j.msea.2004.08.030
中图分类号
TB3 [工程材料学];
学科分类号
0805 ; 080502 ;
摘要
Casting experiments were carried out to produce gray cast irons with compositions in the range (wt.%): Fe-3.2C-wCu-xMo-yMn-zSi, where w = 0.78-1.79, x = 0.11-1.17, y = 0.68-2.34 and z = 1.41-2.32. These key elements were varied systematically during sand casting into 30-mm diameter bars to assess their influence on the development of microstructure and mechanical properties. It was found that microstructures ranging from fully pearlitic to an intimate mixture of retained austenite and bainitic ferrite, termed ausferrite, were produced and a reasonable linear correlation was observed between ausferrite volume fraction and strength. The optimum combination of mechanical properties was achieved in an alloy of approximate composition Fe-3.2C-1.0Cu-0.7Mo-0.55Mn-2.0Si, which generated 100% ausferrite without alloy carbides. This alloy has a microstructure and mechanical properties comparable to austempered gray iron without many of the problems associated with austempering. (C) 2004 Elsevier B.V. All rights reserved.
引用
收藏
页码:326 / 333
页数:8
相关论文
共 50 条
  • [31] Effect of cerium on the as-cast microstructure of a hypereutectic high chromium cast iron
    Qu, Yinhu
    Xing, Jiandong
    Zhi, Xiaohui
    Peng, Jiyun
    Fu, Hanguang
    MATERIALS LETTERS, 2008, 62 (17-18) : 3024 - 3027
  • [32] Effect of potassium on as-cast microstructure of a hypereutectic high chromium cast iron
    Liu Qing
    Yang Hua
    Ding Haimin
    Zhang Tian
    CHINA FOUNDRY, 2011, 8 (02) : 202 - 206
  • [33] Effect of Si on the microstructure of eutectic cementite in as-cast malleable cast iron
    Zhou, Rong
    Lang, Benzhi
    Wu, Yongsheng
    Zhuzao/Foundry, 1997, (01): : 21 - 24
  • [34] Effect of potassium on as-cast microstructure of a hypereutectic high chromium cast iron
    *Liu Qing1
    2.School of Power and Mechanical Engineering
    ChinaFoundry, 2011, 8 (02) : 202 - 206
  • [35] Influence of Sn and Nb additions on the microstructure and wear characteristics of a gray cast iron
    Qiangguo Li
    Yanan Zhang
    Yaning Zhang
    Haibo Liu
    Haonan Ren
    Yamei Zhong
    Xuefei Huang
    Weigang Huang
    Applied Physics A, 2020, 126
  • [36] Influence of Primary Austenite Dendrite on the Microstructure and Mechanical Properties of Gray Cast Iron
    Zhang, Juntao
    Ren, Fengzhang
    ADVANCED ENGINEERING MATERIALS III, PTS 1-3, 2013, 750-752 : 450 - 453
  • [37] Influence of Sn and Nb additions on the microstructure and wear characteristics of a gray cast iron
    Li, Qiangguo
    Zhang, Yanan
    Zhang, Yaning
    Liu, Haibo
    Ren, Haonan
    Zhong, Yamei
    Huang, Xuefei
    Huang, Weigang
    APPLIED PHYSICS A-MATERIALS SCIENCE & PROCESSING, 2020, 126 (04):
  • [38] MEASURING STRENGTH IN GRAY CAST-IRON
    JANOWAK, J
    MODERN CASTING, 1985, 75 (03) : 39 - &
  • [39] BENDING STRENGTH OF GRAY CAST-IRON
    NOGUCHI, T
    JOURNAL OF TESTING AND EVALUATION, 1990, 18 (01) : 70 - 75
  • [40] Effect of alloying elements W, Ti, Sn on microstructure and mechanical properties of gray iron 220
    Abdul Razaq
    Jian-xin Zhou
    Talib Hussain
    Zhi-xin Tu
    Ya-jun Yin
    Xiao-yuan Ji
    Gen Xiao
    Xu Shen
    China Foundry, 2019, 16 (06) : 393 - 398