A series of (Sn0.8Pb0.2)(1-x) Mn (x) Te alloys with x = 0, 0.03, 0.06, 0.09, 0.12 and 0.15 were prepared by melting, quenching and spark plasma sintering (SPS) techniques to investigate their phases and thermoelectric properties. Mn was used as doped element in Sn0.8Pb0.2Te solid solution to reduce the carrier concentration, enhance the Seebeck coefficient and reduce the thermal conductivity of the material. Experimental results show that the SnTe-based solid solution single phase was formed in the alloys with x = 0 and 0.03. The minor irregular-shaped MnTe2 phase presents in the alloys with x a parts per thousand yen 0.06, while the minor needle-like MnTe phase appears in the alloys with x a parts per thousand yen 0.12, together with the SnTe-based solid solution matrix. The lattice parameter a of SnTe-based solid solution decreases nearly linearly as Mn content x increases up to 0.12, but keeps constant as x further increases. All the samples show p-type conduction. Mn doping in Sn0.8Pb0.2Te decreases its carrier concentration and thus increases its Seebeck coefficient. The solute Mn and Pb atoms in the SnTe-based solid solution, and the minor phases MnTe2 and MnTe, enhance the phonon scattering and thus reduce the thermal conductivity. As a result, the figure-of-merit ZT of the (Sn0.8Pb0.2)(1-x) Mn (x) Te composites can be enhanced with proper Mn substitution. The maximum ZT of 0.65 was obtained in the sample (Sn0.8Pb0.2)(0.88)Mn0.12Te at 723 K, which is higher than the 0.29 of its parent alloy Sn0.8Pb0.2Te.