The formation and stability of the L1(0) phase in Mn-Ga binary alloys with compositions in the range 50-75 at% Mn (in steps of 5 at%) has been studied. Of these, single-phase L1(0) structure was successfully produced in the 55,60 and 65 at% Mn alloys by annealing the high temperature phases, which had been I etained to room temperature following arc melting. Further annealing and thermal analysis were used to determine the phase transformation temperatures in the alloys and the results were used to guide further processing. The saturation magnetisation, M-s, and the anisotropy held, Fl, were determined in applied fields up to 14 T. For Mn55Ga45, mu M-0(s)=0.807 T and mu H-0(a)=4.4 T were observed. Mechanically milled Mn55Ga45 powder had coerciviLy of mu H-0(0)=0.393 T, which was a twentyfold increase compared to the bulk material but the magnetisation was reduced (cf. powder: mu M-0(5 T)=0.576 T, bulk: mu M-0(5 T)=0.780 T). Annealing the powder at 400 degrees C led to recovery of the magnetisation but reduced the coercivity, which was still 10 Limes as high as the bulk value. A degree of texture of 045 was achieved by magnetic alignment of the powder particles, leading to a remanence of 0.526 T. Furthermore, isotropic hot compacts of powders were produced with packing density from 83% to 99%, in which the improved coercivity of the powders was partially retained. (C) 2015 Published by Elsevier B.V.